Completely stain red oak wood

5/8/22       
Michael R Member

I need advice on how I can completely stain red oak wood BLACK. I have been using General Finishes black oil gel stain and the only way I can get the red oak wood completely black is by applying 4 to 5 coats. What am I missing? Is there a way I can get the red Oak black without spending so much time and money?

I don't want to paint it black and with so many coats of primer essentially hiding the oak grain.

Thank you, group!

5/8/22       #2: Completely stain red oak wood ...
Mastercabman

If you want it black..
Paint it black...!

The grain will still show!

5/8/22       #3: Completely stain red oak wood ...
Pete

I would use 2 part wood bleach. Neutralize with vinegar. Try your gel stain or go with an alcohol dye.

5/8/22       #4: Completely stain red oak wood ...
Michael R Member

Pete, Just so that I am absolutely clear about what you are saying.
Use 2 part wood bleach with water
THEN use STRAIGHT vinegar to neutralize the bleached oak wood
THEN use the General Finishes Gel Stain???

5/8/22       #5: Completely stain red oak wood ...
Pete

I use a 2 part wood bleach where you mix part A and B. Apply that directly to the oak with out any extra water. Let it sit for a night. This takes the red out. I then neutralize the bleach with thined out vinegar. I'll mix maybe 10 parts water with 1 part vinegar. Maybe someone else can chime in on this water to vinegar ratio. Im guessing your gel stain will do what you want color wise after you get out all the red. With using bleach and vinegar, I know you can have some issues with your top coat. I have used shellac and regular nitro lac over it without issues. Your pre cats and cats may have issues but may not if you use a vinyl sealer...

5/8/22       #6: Completely stain red oak wood ...
Michael R Member

I'll probably just paint it black because I don't want any problems with my water-based lacquer finishing. I switched from solvent-based lacquers a few years ago.

You know it's funny I did a project like this a few years ago without any problems but the difference was I used white oak. I guess I'm getting old. I'm going to do a test sample tomorrow just using white oak and if that does the trick. If so I'll just go get four sheets of the white oak.

5/8/22       #7: Completely stain red oak wood ...
RichC

Black leather dye is what I use for a hard black dye. Many dyes end up with a bit of blue showing under direct lighting.

5/8/22       #8: Completely stain red oak wood ...
Leo G Member

Black dye. Black stain, clear coat, black toner, clear coat.

If you can find a black based on green it would be better than a black based with blue because it will kill the red in the oak.

5/12/22       #9: Completely stain red oak wood ...
Dave Edgerton  Member

I agree with Leo. It's the only correct way and that is how we do it. Solvent based black dye, not water based

5/21/22       #10: Completely stain red oak wood ...
Sean

I would just stain is black, thin my sealer 100%, 1 coat to lock in. Scuff with fine sanding sponge. Make a shader.....1 ounce or 2 TBL Lamp Black 844 IC, 10 ounces of sealer, then 20 ounces lacquer thinner (1 quart formulae). Shade everything, not tone, shade.......until straight black. Seal 2 passes with the thinned sealer. Now you are black with hardly any film build. Add the Lamp black to your topcoat to make a toner the topcoat like normal. This would be my approach for a solvent system.

5/21/22       #11: Completely stain red oak wood ...
Michael R Member

Sorry group I was out of touch since I originally posted my question until now. I just read Leo's and that's exactly what I did last week and the customer approved my sample. I put General Finishes black gel stain over Gen. Finishes black dye and it turned the red oak black. I finished the sample with clear coat lacquer and it really came out sharp. Not a lot of effort but I did prep the sample with 120 and 150 sandings then I water dampened to raise the grain then sanded 220 and 320 then I applied the black dye and black stain following with clear coat.

5/21/22       #12: Completely stain red oak wood ...
Adam

We used MLC Woodsong solvent based black dye/stain to do an entire downstairs white oak flooring of a large high end house.. That was about 20 years ago. It was very black.

Woodsong is a very good product.

12/12/22       #13: Completely stain red oak wood ...
Jon W Member

There are many options:

Spray stain - black NGR dye with pigment. about 3oz 844 LB plus a couple hundred ml of NGR Black per quart. If not penetrating into the deep grain, then cut your stain base with xylene to extend the dry time.

Wipe stain - Water pop, then 8oz 844 LB per quart, if you have a good stain base that can take dyes then add 100 ML or so of Black NGR.

You can also wipe stain black, then spray some black NGR over top after the wipe stain dries to to get it to fully cover. It will look blue till you seal it.

You can also add some black NGR to your sealer coat for extra blackness.

Gel stain should be unnecessary.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production

    Become a Sponsor today!