I have been having some trouble with top CV wrinkling over areas that are filled with various wood fillers...
What is your go-to filler for cracks/ joints under conversion varnish?

I've triedthe following:
-Titebond II (and III) mixed with sanding dust but it dries too slowly.
-DAP Plastic Wood wrinkled on some (even when left to dry overnight).
-Bondo All-Purpose Putty and Minwax High Performance Wood Filler were okay but not long enough 'open time' for filling multiple doors.
-Regular old Minwax Stainable Wood Filler was too course and just got sanded out of small cracks...
-We used CA Glue (Titebond and Starbond) but that is expensive with the glue and accelerator.

Any others we should try?
Thanks in advance.
-JJE

8/16/23       #2: Wood filler for Conversion Varnish ...
RichC

You might want to post the brand and if it's acrylic or solvent based CV.

8/16/23       #3: Wood filler for Conversion Varnish ...
Joe Eberle Member

We use solvent-based ML Campbell Turino.

8/16/23       #5: Wood filler for Conversion Varnish ...
RichC

Famowood is my go to.

8/17/23       #6: Wood filler for Conversion Varnish ...
Leo G

Elmer's E849D8 Carpenter's Interior Wood Filler, not the stuff with wood fibers which is too coarse and not smooth and creamy.

Bondo or equivalent for larger areas

CA glue with an accelerator for some but rare for me.

8/17/23       #7: Wood filler for Conversion Varnish ...
Bart

Haven't used it under CV but I've been using Timber Mate for years. They all shrink, even bondo. The best bet is to let them all cure over night. More cure time is always better. Not sure what coat you're filling but I would never fill before the last coat.

8/18/23       #8: Wood filler for Conversion Varnish ...
Adam

The number 1 thing people don't get with filler is the hardness. If the filler doesn't match the surrounding substrate you will get telegraphing. Mixing glue with sawdust is generally much harder than wood. Bondo is likewise harder than wood. It also eventually shrinks, unless you leave a lump for a week to cure then sand it.

If you are doing paint grade the best method is to use a filler that matches the primer coat.

We use Zar & Timbermate.

8/20/23       #9: Wood filler for Conversion Varnish ...
duster

Another vote for Timbermate. It shrinks less than anything else we've tried. No compatibility problems with precat or CV.

8/21/23       #10: Wood filler for Conversion Varnish ...
Joe Eberle Member

Alright, Im going to try the Timbermate and Famowood... I will report back after I run them through their paces.
Thanks everyone for your help.
I appreciate it.
-JJE

8/21/23       #11: Wood filler for Conversion Varnish ...
Bart

The Famo solvent absolutely shrinks more than TimberMate and IMHO doesn't dry as hard and seems to be more porous. Plus it drys up in the can beyond salvage if you don't use it for awhile. I've got a jar of 3yr old white TM still working fine.
my2cts
Cheers

8/21/23       #12: Wood filler for Conversion Varnish ...
Joe Eberle Member

Much thanks, Bart!
-JJE

8/21/23       #13: Wood filler for Conversion Varnish ...
RichC

Famowood absolutely does not dry beyond salvage. First you keep the lid on tight and the rim clean. When you notice it getting dry, add some lacquer thinner in the can and the next day it's like new. If you don't touch the can for a year and let it become a rock, then you still add lacquer thinner but wait a couple of days. I guess I don't know just how big of crack is being filled. If it's bigger than hairline, then I make a new part. Famowood does not shrink much if you are filling hairline cracks. I always overfill a bit and then sand it flush when it's dry anyway.

8/21/23       #14: Wood filler for Conversion Varnish ...
Bart

Come on Rich. Been there done that. If I'm doing stain and clears that don't match the Famo color I might not open a can for months. I can't tell you how many partials I've burned through. Is what it is.

TimberMate has them over a barrel for life expectancy and quality.
Cheers
Bart

8/22/23       #15: Wood filler for Conversion Varnish ...
RichC

It's your choice to let them go rock hard Bart, but not everyone chooses to do that.

8/22/23       #16: Wood filler for Conversion Varnish ...
Leo G

Timbermate comes in a glass jar, right? Probably a much better seal than the metal can which is why Famowood goes hard after a while even in a sealed can.

I find Famowood to be too hard sanding for just filling holes. If you need to put a screw or fastener in it that's where it might shine.

8/22/23       #17: Wood filler for Conversion Varnish ...
Yavuz Member

Elmer's E849D8 all day long. No shrinking,no compatibility issue,fastest drying and smooth as silky sanding .Conversion Var. or PreCat Lac. or any 2k polys.
One can argue but trying is believing. I suggest order from Amazon and give it a try.
Good Luck !


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production

    Become a Sponsor today!