Metal Laminate Over 1/2" Mdf Fail

2/6/21       
Geoff

I made an open cabinet with a 4' x 4.5' x 1/2" mdf back. Prior to putting on the back I laminated metal laminate with contact adhesive to it. One coat of glue on laminate and two coats on mdf. The bond seemed fine but now some bubbles have appeared.

I did the sides the same way but with 3/4" mdf and no issues.

I should also mention the 1/2" back developed a significant bow. Convex toward the laminate side.

Looking for advice on repairing the back. Although I think that is wishful thinking. I do have access to a vacuum press(?).

If I have to remake the back should I laminate both sides? Anything else?

Geoff

2/7/21       #2: Metal Laminate Over 1/2" Mdf F ...
Thomas Gardiner

Ignore balanced layups at your peril. By applying glue and laminate to one side only you have possibly, introduced moisture from the glue and inhibited the absorbsion/evaporation of atmospheric moisture from the substrate on one face only. It is the winter so likely the substrate has a high relative humidity coming from the stack of freshly manufactured mdf and wil subsequently lose humidity in the low relative humidity of the heated shop. So the mdf shrunk (shrank?) but the laminate has captured the one face dimensionaly. That is why you have bubbles of localized glue failure due to shear stress and also the convex panel.
can you fix it? Probably not but you could try. I have had limited success with misting a concave surface with water and waiting until the surface is dry before glueing. The warp is reduced but not eliminated. You have a vacuum bag so you could apply a backer laminate with PVA in the bag. This is closer to a balanced layup and will do double duty of swelling the back of the panel with glue moisture. Don't expect miracles but it might work.
You still have the bubbles to deal with. Until you flatten the panel don't try to fix the bubbles. If you get a flat panel after applying plam to back then you can first try a hot iron on the bubbles to reactivate the contact cement and roll out the area. Test that the iron won't ruin the laminate on some scrap.
I have heard of but not tried drilling from the back and injecting glue under the bubbles then pressing in the vacuum bag.
Good luck. Now you know what not to do next time.

2/7/21       #3: Metal Laminate Over 1/2" Mdf F ...
Geoff

Thank you. What you said makes total sense. Knowing what to do next time is going to be happening sooner then later.

2/26/21       #4: Metal Laminate Over 1/2" Mdf F ...
bill

In addition to moisture you created a bi-metallic strip situation. The lamainte is going to expand and contract with changes in temperature.

Again the solution is a balanced panel. I think we all do that once.....

3/28/21       #5: Metal Laminate Over 1/2" Mdf F ...
Geoff

I haven't been back here for awhile...

I remade the panel pretty much right away.

My project manager was mad and tried to get me to redo the work off the clock. He is new to our company and was informed that this is not company policy. I clocked in under "warrenty" work and we don't charge the cllient for replacement material (This project happens to be "Time and Material")

Anyway, I laminated the back with a basic solid color plastic laminate (Formica) and the exposed side with the metal laminated and the panel stayed flat and no delaminations.

Success!

Thanks,
Geoff


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Today's Sponsors
    • NEMI
      Products For CNC Machines - Digitizers, Tool Setters, Vacuum Pods, Vacuum Cups, Vacuum Tables, Vacuum Chucks and Software
    • Southeast Tool, Inc.
      High Quality Tooling at Competitive Pricing
    • Cab Parts
      Pre-manufactured Components for Easy-to-Assemble Cabinet Boxes
    • Parts Cutter CNC
      CNC Cabinetry and Closet Parts
    • Western Dovetail
      Custom Made Dovetail Drawers
    • TradeJobPlacement.com
      Individualized Placement Services, Specializing in Millwork Design Engineers
    • iBiDMachinery
      The Nation's #1 Used Woodworking Marketplace - Buy and Sell Woodworking Equipment with iBiD!
    • 360 Degree Machinery
      Specializing in high end American, European, and select Import woodworking machines.
    • MARTIN Woodworking Machines Corp.
      Quality Woodworking Machinery Engineered and Manufactured in Germany
    • VortexTool Co. Inc.
      Manufacturers of Custom Cutting Tools, and Distributors of Major Cutting Tool Brands
    • RT Machine Co.
      Stocking Distributor of New and Used Woodworking Machinery
    • Centex Automation
      New and Used Machinery sales and service
    • TradeSoft
      Seamless Management Software to Improve Estimating, Job Costing, Scheduling, Purchasing, Shipping, and Shop Floor Data Collection

    Become a Sponsor today!