drying to single digits p2

1/7/16       
Kim Vedros  Member

Website: http://www.archturnings.com

I've built my insulated chamber and have a dehumidifier coming in. My question is what variables to use (temp, time and RH) to get my 6/4 and 8/4 red oak from ~10% MC to ~7% MC.

1/7/16       #2: drying to single digits p2 ...
John Member

I run my home built dehumidification kiln at 110F and follow a drying schedule like shown below. When the extraction rate falls off to 25% of the first day, I move to the next lower RH.

10% MC; 60% RH
9.2% MC; 55% RH
8,4% MC; 50% RH
7.5% MC; 45% RH
6.7% MC; 40% RH

So if you want 7% MC for your final value, make the last setting about 42% RH.

John

1/8/16       #3: drying to single digits p2 ...
Kim Vedros  Member

Website: http://www.archturnings.com

Thanks John
How long do you think to get 6/4-8/4 red oak from 10%MC to 7%

1/8/16       #4: drying to single digits p2 ...
Kim Vedros  Member

Website: http://www.archturnings.com

So I guess it wouldn't be advisable to set to 40% RH when I'm at 9-10%MC

1/8/16       #5: drying to single digits p2 ...
John Member

It's impossible to say how long it will take to dry from one MC to another. It depends upon how much lumber is in the dryer, how much water the dehumidifier can process per day, and quite a few other factors. In my kiln with a full load of about 275 BF operating at 110F with a 40 pint/day dehumidifier, it takes about 12 - 15 days to go from 12 - 14% starting MC to 7% for 4/4 and 5/4 stock, so call it 2 days / % water removed.

No don't set the kiln at 40% when your lumber is at 9 - 10% MC, follow the chart and set it at 50% until it gets close to 8.4%, then set it to 45%, etc. Small changes, not big ones, especially when drying 8/4 stock and difficult to dry woods like white oak.

John

1/9/16       #6: drying to single digits p2 ...
Gene Wengert-WoodDoc

At 60% RH, the lumber's surface will dry to about 10% MC, but no drier. It will take many weeks to get that dry throughout the piece. So, the surface will be at 10% MC, but it is impossible to get the surface any drier. The core will therefore be wetter.

To achieve 7% MC lumber in a reasonably short time, you will need to use 25 to 30% RH or a bit lower at 110 F. That will give 6% MC at the surface.

As a rule of thumb, at 110 F and 30% RH, you might, on a good day, achieve with 4/4 oak about 1/2% MC loss per day. For 8/4 less than 1/4% MC loss per day. Why so slow? We are waiting for the water to move out of the wood and not for the air to scrub the water off the surface. So, the size of the compressor is not the issue at these low MCs, but rather how fast the water moves out of the wood. Temperature is a big factor at the end of drying. If the surface MC and the air's moisture are the same (such as 60% RH and 10% MC), then no drying will occur.

A complete listing of RH and MC values is given in many documents, including pages 16 & 17 in DRYING HARDWOOD LUMBER. (Download here at WoodWeb.)

1/9/16       #7: drying to single digits p2 ...
Kim Vedros  Member

Website: http://www.archturnings.com

Thanks Doc. I found your chart. I purchased an Ebac LD800 and the sparse info in their manual says not to increase temp more than 5deg Cent. per day. Not sure if damage to the wood should be expected when it is already down to 9-10%MC.
As for temp. the unit should go well above 110d

  • Post a Response to this thread
  • notify me of responses to this topic
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)