uneven cut on bandsaw mill

10/17/14       
Assar

I have been operating a manual bandsaw mill, sawing a variety of woods in varied diameters and lengths. Regardless of the wood I'm sawing I find that the blade tends to dip on the first 12 inches of the cant before it levels off. This makes for curved ends of boards which I have to cut off. I have tried moving the logs further down the mill and the cuts are the same. The dogs are doing their job and the logs don't lift off the bed while sawing. Does anyone have tips on how to avoid this?

10/17/14       #3: uneven cut on bandsaw mill ...
Tennessee Tim

Website: http://www.tsmfarms.com

Sounds like dull blade(s)...Also Cooks sawmill website has a great info section on setting up a band correctly......it done wonders for my saw....I highly reccomend doing this to ANY brand bandmill.

Which saw do you have??? what is the cutting width between guides??

10/18/14       #4: uneven cut on bandsaw mill ...
ron v

Check the alignment of your blabe in relation to the bed of the mill. Sounds like your blade may actually be pointing domnward to begin with. Look at the boards you cut. If they have rob marks on them then the blade is not traveling straight.in your case there would be rub marks on the bottom face of the board as it comes off the mill.

10/18/14       #5: uneven cut on bandsaw mill ...
Rod Hays

here is how i check to see if the blade is running level with the bed. i use a 2 foot level placed on the blade,then i measure each end of the level to the bed to see if the measument is the same. if not then i adjust till they are the same distance. on my bandsaw mill i adjust the band wheels to get the blade to run level with the bed.

10/19/14       #6: uneven cut on bandsaw mill ...
Assar Member

I have leveled everything several times, but I will check this again. I can't see why it would only dip at the beginning of the cut and then level off...and that is regardless of which bunk I start the cut on. No rob marks that I have noticed. But it does make sense that the blade might be tilting down somehow, at least at the start.

10/20/14       #7: uneven cut on bandsaw mill ...
Eric

How fast are you feeding the saw at the start of the cut? And what is the thickness of your bandsaw blades?

I get this kind of behavior when my blades are dull and I feed the saw too fast. It's worst at the start of the cut, when the blade isn't "in" the wood yet.

If you are not using a heavy gauge thickness on your blades, or if they are not very sharp, you can get this behavior.

A sharp blade will not rise or dive in a cut at almost any feed rate, so check that first.

10/20/14       #8: uneven cut on bandsaw mill ...
assar

Nope, it's not the blade. Brand new blades and re-sharpened blades behave exactly the same. I try and start the cut really slowly, but this is tricky to do isn't it? Sometimes I cut about an inch and then back off and start again and this seems to help a little.
I'm fairly new to bandsaw milling. I used to use a chainsaw which cut just fine amidst the noise fumes and dust. I much prefer the bandsaw, but I do find that it doesn't like knots in softwood. Aside from my problem with the first foot, the cut gets wavy when I am cutting in soft woods with knots. Dryer hard woods seem to cut smoothest.

10/20/14       #9: uneven cut on bandsaw mill ...
Rod Hays

could be your blades guides. i set my guides so there is no play in them. if the blade is sharp,running level with the bed and the blade guides are doing there job,band wheels don't have any play and the blade is tracking right it should cut without any waves.

10/20/14       #10: uneven cut on bandsaw mill ...
assar

Rod, No play? Does that mean that they are up against the blade and spinning all the time?

10/20/14       #11: uneven cut on bandsaw mill ...
Rod Hays

yes

10/30/14       #12: uneven cut on bandsaw mill ...
Tom the Sawyer  Member

Website: http://www.TomTheSawyer.net

Assar,
If your blade is level and sharp, watch the RPMs closely to see if they vary in correlation with your cut changing. Also check your belt tension.

12/26/14       #13: uneven cut on bandsaw mill ...
old 243

I have had to get my blade guides squared up on a lathe and a bit taken off the front as they wear. This keeps the blade supported an d running true. Also if you are cutting softwood you might need a little more set in your blades, as you come to a large knot , I will reduce the feed speed as you go from soft to harder wood this will reduce some dip. Sounds to me that you have adjustments or corrections to make on your guides or guide bearings. Milling is a long learning experience, have fun.

3/16/17       #14: uneven cut on bandsaw mill ...
Todd Goodness  Member

I have had this happen to me with frozen pine logs with heavy knot sections. Also if its a butt log the first few feet from the bottom up are considerably harder wood. That density along with variable other issues like under tensioned blade, wrong set ,feed to fast,,blah blah...Has always seemed more of a problem to me in the winter months.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • Rose Machinery
      Horizontal Band Re-rips, Standard & Custom Designed Machinery
    • Baker Products
      Industrial Woodworking Machines, Wooden Pallet Manufacturing Machines, & Portable Sawmills

    Become a Sponsor today!