5/18/20       
Tommy Hart

We have an American Bandsaw Mill, with which we have been cutting hardwood logs for the last 12 years.

Unfortunately, this last week, we have been breaking bandsaw blades very quickly. Usually we get 3 to 4 sharpenings out of the blade before it breaks.

This past week we are breaking new blades on the first cutting.

If anyone could shed some light as to why this is happening, we would greatly appreciate it.

Thanks,

Tommy

5/18/20       #2: RE: Bandsaw blades breaking ...
Tommy Hart Member

To the original post....

I just wanted to add that the bandsaw mill is a relatively large horizontal sawmill with a band blade of 19' 6" and has 30" wheels.

Also, it has a powerful 86 hp Cummins diesel engine which can handle logs of 30" to 32" in diameter, and 21' long.

5/19/20       #4: RE: Bandsaw blades breaking ...
Jim Member

Are they breaking at the weld?

5/19/20       #5: RE: Bandsaw blades breaking ...
Tommy Hart Member

The blades are breaking in random areas, but not at the weld.

5/20/20       #6: RE: Bandsaw blades breaking ...
Mark Hineman Member

It sounds like you are sharpening the blades yourself.
As I understand "micro fractures" occur at the bottom of the gullet. If your setup includes a well dressed grinding wheel, and you are getting a good grind at bottom of the gullet, it should clean up those fractures.
Otherwise the fracture continues and the blade breaks

5/20/20       #7: RE: Bandsaw blades breaking ...
Mark B Member

If your blades are breaking brand new and not at the weld would assume youve checked all the usual suspects, blade tension is correct, guides are correct, operator is not slamming into the end of the log, not crowding/over feeding, and so on. Outbound of that I would be contacting your blade supplier or trying a few blades from a different supplier to see if somehow you got a bad batch of blades which would seem odd.

Ive read and been a part of a bunch of conversations pertaining to what Mark mentions about micro fractures but you say they are breaking on the first go with a brand new blade. That wouldnt really pertain to re-sharps. I always grind/ground our full profile (hook, rake, and full grind on the gullet) to address the micro fractures but I know a ton of guys who sharpen, or have their blades professionally sharpened that may only grind the hook face or the hook face and the top of the rake and swear they have never had an issue. I prefer the full grind but given the experience others mention and the speed of not grinding the gullet who knows.

Theres not a lot of factors if its happening with new blades. Blade material, mechanical issues, or operator error.

5/31/20       #8: RE: Bandsaw blades breaking ...
GeneWengert-WoodDoc

I assume that you have the correct width of blade for your machine. If you are breaking a blade at random places, either the blades are junk or you have way too much tension. Normally, feeding to fast would stall the motor,

6/9/20       #9: RE: Bandsaw blades breaking ...
Eric Steadle

If it was working well, and now it's not, something changed. If it's not the bands (new supplier, etc.) then look for what else may have changed. Consider that something may have broken or failed.

Examine the tracking plate closely on the idler wheel... you may find that it has weakened, or one of the hinges has broken. Perhaps it was bumped by a machine and knocked out of true by a log.

Check for loose or perhaps broken bolts that fasten the tracking plate to the frame. Also check that the idler wheel bearing is spinning freely. These are often "sealed" bearings and they have a lifetime. After a couple 1000 hours you'll need to replace it.

On the drive side, check the main bearings and ensure they are rotating freely, the shaft is true and not bent. Check the grease fittings (usually dashpots) and make sure they are pushing grease into the bearings.

After all that, check your bandwheels to ensure they are co-planer. Lay a straight metal level or ruler horizontally across the face of the bandwheels about 1/3 of the way down from the top, and above the axle. Look closely at the 4 outer edges of the bandwheel that touch the straight edge, and check for any gaps between them. Do this again below the axle 1/3 of the way, and check again.
If you find any gaps, you should adjust the bearings or the tracking plate to get them dialed in. If bandwheels are not perfectly co-planer, the band stretches unevenly from front to back as it rides around the wheels and those stresses will cause metal fatigue more quickly than normal. Sometimes you can look at the blades and see very slight cracks in the other gullets of a failed blade, or on the backside of the blade working its way toward the gullet. If you see this in your broken blades, it's a sign that the bandwheels are not co-planer and need to be adjusted.

Also check your roller guide bearings and make sure they are not seized. (You'd probably have noticed that as they tend to scream when they won't turn.)

Post a picture of your broken edges of the blade and someone can probably tell whether it broke because of stress fracture or from fatigue. That will help narrow it down at least.

Best of luck to you.

12/22/20       #10: RE: Bandsaw blades breaking ...
Rooster Member

Tom do you get any push off or diving on the end of cuts could be out of square blade guides putting stress on your blades I have a woodmizer Lt 70 or blade too far away from the bearing shoulder


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • Baker Products
      Industrial Woodworking Machines, Wooden Pallet Manufacturing Machines, & Portable Sawmills
    • Rose Machinery
      Horizontal Band Re-rips, Standard & Custom Designed Machinery

    Become a Sponsor today!