Veneer

You are not logged in. [ Login ] Why log in
(NOTE: Login is not required to post)

Post a Response
The staff at WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at any WOODWEB Forum. Participants should undertake the use of machinery, materials and methods discussed after considerate evaluation, and at their own risk.
Your Name:
Your Website:
Email Address:
Subject: Re: wrinkling in veneer....causes?

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

wrinkling in veneer....causes?

11/25/15       
Dan Cook

I vacuumed 2 cherry tops the other day and both came out with wrinkling in the veneer. I am wondering what possible reasons would cause this. It was raw veneer glued with cold press glue and clamped in a flat bed vacuum press. There was plenty of pressure and I didn't have problems with other veneer layups, only this cherry. Suggestions?

11/25/15       #2: wrinkling in veneer....causes? ...
Max Neu

I would guess too much glue.

11/25/15       #3: wrinkling in veneer....causes? ...
howard Member

Did you have a platen on top of the veneer that is rigid enough so it lays completely flat as the bag squeezes down on it? If there were too much glue, this would help to push it out the sides. Another thing, if the veneer itself is not flat and you are not using a platen, the bag itself will not necessarily push all the unevenness out.

11/25/15       #4: wrinkling in veneer....causes? ...
Joel

To add to what Howard said, Wrinkling is caused by insufficient top pressure. Any give in your top platen will allow the veneer to wrinkle up. Any uneveness in the thickness of the veneer will allow the low spots to wrinkle. For my silly little layups I use sheet cork to take care of this problem. For a 4 by 8 sheet i'll bet there is a rubber membrane used in industry.

11/26/15       #5: wrinkling in veneer....causes? ...
Dan cook

Because I'm using a flat press I am using the bottom platen to press down against the table. This works fine and never have had this problem before...only this cherry. I was doing a border veneer around the perimeter and the ends had the grain running perpendicular to the field. I am suspecting that may have not let it expand so I'm relaying up the top without the border and will let you know if that is the culprit. Here is a picture of the small top. The larger one was the worst.


View higher quality, full size image (640 X 480)

11/26/15       #6: wrinkling in veneer....causes? ...
Dan cook

Because I'm using a flat press I am using the bottom platen to press down against the table. This works fine and never have had this problem before...only this cherry. I was doing a border veneer around the perimeter and the ends had the grain running perpendicular to the field. I am suspecting that may have not let it expand so I'm relaying up the top without the border and will let you know if that is the culprit. Here is a picture of the small top. The larger one was the worst.


View higher quality, full size image (640 X 480)

11/26/15       #7: wrinkling in veneer....causes? ...
Joel

It is unclear from your pick where the wrinkling is. I press stuff with the veneer going in all sorts of directions and have never had a problem. Is the wrinkling in the vicinity of the black and white border? If so then these veneers are thicker leaving the cherry room to wrinkle. It doesn't take much. I guess it could be too much glue like Max says but it would have to be way too much. When I use to much glue it just bleeds thru.

11/26/15       #8: wrinkling in veneer....causes? ...
Dan Cook

Ironically the wrinkling happened inside of the border on both sides. It went in about 4' and length of about 10". Because I had laid it up with the border all as one I thought maybe the veneer going across the end might have kept the piece from expanding under the pressure. There was no bleed thru and I didn't spread the glue any more than normal. Anyway I started over again with a new sheet and didn't do the border, which i will do in a second step and this time no problem.

11/26/15       #9: wrinkling in veneer....causes? ...
rich c.

What's the substrate? Was it dry? Is that frame around the outside solid wood, or veneer? What thickness of veneer? Was the glue fresh?

11/27/15       #10: wrinkling in veneer....causes? ...
Dan cook

Thanks to all who responded. I think I've located the problem. I used a solid wood edge which I rabbeted into a particleboard panel. The top, including the stringing was all done in veneer which overlaid the hardwood edge. Only a 1/4" of hardwood came to the top due to the rabbet. I think what happened was the stringing was a few thousandths thicker than the surrounding veneer and thus the pressure from the vacuum was not getting through to the field. This I determined because I had a lot of loose spots on the outside edge as well. I'm making a new top now and have already laid the field which came out fine...no wrinkles. I'm going to do the edge the same as before but in a separate pressing. Also I'm going to put felt between the platen and the veneer for the differentiation between the stringing and the veneer. I made the stringing by making a hardwood sandwich and then cutting thin strips from it. I used a micrometer on the veneer and the stringing and the stringing was about .003" thicker than the veneer. Just barely enough to feel, but apparently enough to cause problems when pressed all at once. I'm working on it today and will let you know how it turns out. No such thing as failure...only experiments to identify what doesn't work!!!

11/27/15       #11: wrinkling in veneer....causes? ...
Max Neu

Dan,
Why don't you just plane the banding down to the same thickness as the veneer?

11/27/15       #12: wrinkling in veneer....causes? ...
Dan Cook

I did try to plane the border down to the same thickness but it blew apart in the planer when I tried. I even tried to run it through the wide belt sander but the sander would not adjust that close. What I did was set up a fence setup on the tablesaw which got me down to .003-.004 of the thickness of the veneer. I laid it up and then used a card scraper to level the stringing down to the veneer level. Not really too hard. I still think the problem was that the stringing being slightly proud of the veneer surface did not allow the pressure of the vacuum to be enough on either side of the stringing. Anyway I'm working on it now and will let you know how it goes.

11/27/15       #13: wrinkling in veneer....causes? ...
Max Neu

I use a Veritas inlay scraper to plane down banding,but a block plane will work. Tape 2 strips of the veneer you are using parallel to each other,then the border piece in the middle,the outer pcs.of veneer will act as your depth stop to give you the same thickness. I think it will be worth the few minutes it will take to shave it down.

11/27/15       #14: wrinkling in veneer....causes? ...
Dan cook

Ok, I laid up the veneer field in one pressing. No problem with wrinkling. I did the border in a second pressing and used felt between the platen and veneer to help with the thickness difference problem. It seemed to work very well as everything pressed up nicely. I took the stringing down with a card scraper which didn't seem to take too long. I will let you know how it turns out after stain and finishing.

1/11/16       #15: wrinkling in veneer....causes? ...
Stephen Knowles

I have had the same trouble with both cherry and mahogany veneers. Although my lay-ups were not as complicated as yours I came to believe the solution was to spray the outside surface with distilled water (lightly) just before it went into the bag so that the veneer didn't ripple from the moisture it picked up from the glue side before I was able to get the pressure on. My results have been flat ever since because it buys me that little extra time by keeping the veneer balanced.

4/22/26       #16: wrinkling in veneer....causes? ...
khoi

Hello All,
I hope this would help people. I have veneered for many years and this last adventure was very puzzling, wrinkles after a cold vacuum press glue up. The veneer was very figured eucalyptus. I have done tons of maple, sapele, all types of burl and never really got any wrinkles (not this bad at least).

I have tried different types of glues, glue applicators, heating up the garage, less glue, more glue. I even changed my trusty old vacuum pump. Nothing worked.

The problem, it turns out is that this veneer loves to absorbing water. The thing that finally worked was this. I had to put another caul on top of my piece that is about the same size into my bag and pressed for 1.5 hours.

Normally I have a the bag, the channeled platen, plexiglass on top the platten to help with glue cleanup, then the board with the veneer faced down on the plexi. Worked all these years.

Now I have the bag, the channeled platen inside, the plexiglass (not needed) on the platen, the board with the veneer (veneer facing up) and another board (melanin) on top. This has worked for many many glue ups with this particular veneer.

Hope that helps anyone. I was going crazy that my system was working all these years.

The veneer is nice but damn.


View higher quality, full size image (5712 X 4284)

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors

    Become a Sponsor today!