Ripsaw versus moulding machine for solid wood panel

2/22/20       
Marc Member

Website: http://www.bizier.ca

Hello everyone,
For several years we have been making laminated wood panels using a glue line ripsaw. We would like now to use our moulding machine to prepare the wood to be glued. Before starting full production we conducted some joint solidity tests which so far have not been conclusive.
We made some test blocks using 8/4 sugar maple (acer saccharum), the moisture content was 6 to 8%. For the test we compared the glued joint created by the glue line ripsaw to the joint made with two types of cutter heads, either, straight knives Tersa style , or a multi knives spiral style. Both cutters had new knives.
In order to test the solidity of the joint, we hammered a wood chisel into the glued joint. Before gluing, we did a dry assembly to evaluate the quality of the joint, which were
impeccable.
The results are very disappointing. As expected, the glued joint in the test block made with the ripsaw never failed. However, the glued joint in the test block made from the moulding machine failed most of the time.
We suspect that the glue is either evacuated from joint when it is pressed or the wood is "glazed" and does not absorb the glue.
We decided to redo the test using slightly dulled knives. The glue line was not nice but the joint did not fail.
Would you have any suggestions to solve this challenge?

2/22/20       #3: Ripsaw versus moulding machine for ...
Leo G Member

Since the ripsaw never failed and is likely much quicker than the molder why would you change?

2/22/20       #4: Ripsaw versus moulding machine for ...
Marc Member

Website: http://www.bizier.ca

In order to keep this thread short, I did not elaborated all the details. We are not abandoning the ripsaw production. The molder production will be complementary.

2/22/20       #5: Ripsaw versus moulding machine for ...
John Member

I never glue machine planed wood without sanding first. The surface after machine planing is scalloped, not truly flat, and the fibers are compressed and won't absorb glue well enough to bond properly.

John

2/23/20       #6: Ripsaw versus moulding machine for ...
Adam

The gold standard for using pva and wood has always been sharp knives on a jointer.
pva likes smooth surfaces and thin glue lines.

I suspect the problem is clamping pressure. You are squeezing the glue out of the milled joint. The sawn surface provides enough space for the glue to not be squeezed out.

PVA glues do not work by “soaking” into the surface. There is a problem with mitered/end grain joints “sucking” the glue out of the joint leaving a “starved” glue line that is prone to fail.

Most of the failures people see with epoxy is not abrading the substrate(wood, aluminum, composite) with 80grit. Also way too much clamping force. Epoxy likes rough surfaces and wide glue lines.

The idea that you need to abrade wood as prep before bonding with pva glues is false.

2/24/20       #7: Ripsaw versus moulding machine for ...
Thomas Gardiner

A couple of years ago this question or a similar question came up and I suggested glue starving of the joint by over-clamping. I decided to do a test of how much is too much clamping. It can't be considered definitive in any way because I only used two short samples of cherry for each of rub joint no clamps,moderate clamps typical of a regular glue up and extreme clamping with heavyduty F clamps at 4" intervals with maximum force.
The conclusion was that there was glue line failure on the rub joint sample but the moderately clamped and extremely clamped samples had mostly wood failures
I think glue starving for PVA is not a factor - remember the ripsawn glue up is using the same clamping.
It's been decades since I read Bruce Hoadley's Understanding Wood. I recall there being a chapter on gluing that was extensive.
The suggestion that the scallops left by the moulder would interfere with the glue bond is intriguing but I suspect unless the moulder is cranked up to maximum feed the scallops would be in the range of .001" or less.
I would like to see if the OP tried passing a sanding block over some moulded staves then gluing and seeing if there is a benefit.
One last thing. Are you gluing the parts immediately after machining in both methods? A delay would allow distortion of the surface however small due exposure of the fresh face to drier conditions.

2/24/20       #8: Ripsaw versus moulding machine for ...
Jessica  Member

Website: finecraftsmanlumber.com

It could be a couple different issues. My first guess is your moulder cannot hold the tolerances for a glue line edge. This could be how well the knives were cut or tolerances on the head and spindle. It could also be your feed rate/speed. Too slow and the wood can glaze over, too fast the knife marks per inch will be too spread not allowing for good contact and not producing a glue line edge. And as someone already mentioned, sharp knives will also help your case. Clamp pressure is also important. Too much pressure will force too much glue into the wood, not leaving enough to fill the bond line. But you also want to make sure you have enough pressure. Another possibility is you are using too much or too little glue, but I doubt this is the case because you are already having success with the rip sawn edges. I put a blog together not too long ago on this exact topic. It mentions glue line edge tolerances and other basics. It's a really quick read, so its worth the read.

Link

2/24/20       #9: Ripsaw versus moulding machine for ...
MarkB Member

RE: Starving a joint from over clamping with PVA....

This topic seems to get beaten to death and Tom also contributed to the post linked. Still wish I could find the article from FWW but every test I have ever seen shows that there is almost no way possible for most shops (even those with air/hydraulic/actuated clamp carriers) to ever starve a joint by over clamping. You could space I-bars as close as they can be operated and put every ounce they will allow on the glue up and likely still technically be under-clamping.

Link to post

2/24/20       #10: Ripsaw versus moulding machine for ...
Marc Member

Hello,
Thank you all for your input. In previous test we did try light sanding and different clamp pressure. The end result was joint failure. In our test we glued immediately after machining. I had a second look at our failed test block, please see pictures, some glue seems to have dry on the surface. Instead of clamping immediately after application of the glue, I wonder if letting the glue "soak" longer into the wood before clamping may rectify the problem?


View higher quality, full size image (2592 X 1936)

2/25/20       #11: Ripsaw versus moulding machine for ...
Jessica  Member

Website: finecraftsmanlumber.com

How long did you wait before performing your test? Did you give the glue enough time to fully cure? Just because it is dry on the surface doesn't mean the glue is cured all the way through the joint. For most PVA glues with normal working conditions, the glue should cure for at least 24 hours before testing. As for the idea of letting the glue "soak" in before applying pressure, I think you might cause some more problems for yourself. This opens up the possibility for the glue to precure before pressure is applied, resulting in a weaker bond. I've heard of people doing that with end grain, but with the sole concept of end grain soaks up all the glue and doesn't leave enough glue to fill the bond line. Just out of curiously, what is the temperature of your shop and the temp of the wood when the glue is applied? This could also be a factor of some joint failures, especially with colder temperatures during winter months. Also, if you could, look at the failed joints and inspect to see if the glue or the wood is failing. The cured glue should be stronger than the wood itself. So if the wood is failing, you will see wood fibers adhered to the bond (goal being 100% wood failure, with this you should only see wood fibers on the bond line). If the glue is failing, you would see little to no wood fibers adhered to the bond.

2/25/20       #12: Ripsaw versus moulding machine for ...
Thomas Gardiner

Excuse my ignorance as I haven't run a moulder but could there be any chance of waxilit contaminating the surfaces?

2/25/20       #13: Ripsaw versus moulding machine for ...
Leo G Member

If you are doing full face glue ups you need to let it dry for a few days and keep the clamps on it for 24 hours.

2/25/20       #14: Ripsaw versus moulding machine for ...
David R Sochar Member

If you would like to pursue the glue soaking in, glazed surfaces, etc. look up the link. It discusses a water drop test that helps you know if the surface is good to glue or not.

Drop a single drop of water on the surface to be glued. Watch to see how long it takes before it soaks into the wood. Surface tension holds it as a drop, but eventually it gives way to the drop soaking in. This is also called 'wetting out' and is critical when gluing large surfaces like in veneering.

Glue Tests

2/25/20       #15: Ripsaw versus moulding machine for ...
Marc Member

Website: http://www.bizier.ca

Hello,
Thank you again for providing additional insight. The glueing environment is the following, the average temperature is 18 Celsius (minimum acceptable following manufacturers recommendation is 15C. ), the RH when dust collector is running is 20% and 40% without, the wood is at room temperature. The joint solidity test where performed 6 hours and 24 hours after gluing. We didn’t use any lubricant during the machining.
We have decided to conduct more test next week. This time, we will test three wood species, run the moulding machine at different speed and do the water test as suggested by Mr. Sochar. Any suggestions for our test will be appreciated.

2/26/20       #16: Ripsaw versus moulding machine for ...
Thomas Gardiner

Hey I just looked at your web address now, I'm just down the river from you in Ottawa.
One thought I had is that the major difference between sawing and milling is the sawn edge will have machine marks cutting across the wood cells. This may allow for better glue absorption. So what may be necessary when sanding after the moulder is to sand across the grain to mimic the saw.

2/26/20       #17: Ripsaw versus moulding machine for ...
Marc Member

Website: http://www.bizier.ca

Thank you Thomas. I will had your suggestion to my next trial run. If you are in the area stop by.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Limtech Industries, Inc. Lamello
    Today's Sponsors

    Become a Sponsor today!