First solar kiln load results

7/15/18       
Carl

I just recently finished drying the first load of 4/4 ash
in the solar kiln I built a few months ago, and thought
I'd share the results and hopefully get some input on
the trial run behavior.

The load is just shy of 400 bd/ft, and all 8 foot lengths,
and was carefully stacked with very dry stickers.

The kiln is based on the Virginia Tech plans, with a
foot print of 14 X 7 feet. I decided to use a hinged
roof/collector setup up and a removable front/low wall.
I have a fairly decent tractor with forks, and wanted
to be able to easily load/unload the lumber, and the
forks allow me to lift the roof and prop it open.

Following the guidelines in the Virginia Co-op Extension
publication:

https://pubs.ext.vt.edu/content/dam/pubs_ext_vt_edu/420/420-030/42
0-030_pdf.pdf

I cut sample boards for monitoring MC rate of loss, and
also cut 1 inch samples from the ends of those boards
for oven drying and determining initial MC of the ash.

The oven dry samples showed the ash coming off the
sawmill at 38-40% MC. Based on off-the-stump MC chart
for hardwoods, this was a bit lower then what the chart
shows for ash (45%), but maybe not surprising - these
were ash trees that had been infected by the eastern
ash borer, and this year was the first year they did
not leaf out. The trees were dropped, the logs end
coated, and the logs were sawn within 4 days of
dropping, with the boards immediately put in the kiln
fresh off the saw.

As per the VT documentation, I cut two 30 inch sample
boards, used the formula to estimate the oven dried
weight of the boards, and put them in the pack so I
could pull them out and weigh them each morning, using
the VT doc formula for calculating current MC of the
sample boards, and applying each board's MC value
against the previous days MC value to come up with
the percentage MC loss.

The VT doc mentions quarter sawn lumber drying slower
then flat sawn - my samples were one of each, and
dried as expected - the quarter sawn board slower.

Below are the readings/measurements I took each
day - the percentage figures represent the percentage
of moisture loss compared to the previous day's reading.
The VT doc listed the max recommended drying rate
for ash at a little over 10% per day, which
became the "target" I was looking for. The MC-
values below are the actual daily MC values for the
sample boards determined by weighing each sample and
dividing the noted weight into the estimated oven
dry weight of that particular sample board
(scale resolution was hundredths of an ounce)

I averaged the readings of the two sample boards
to arrive at the single values below, and rounded
to nearest whole numbers. Days with no comments
indicate good sunny drying days.

Day 1 12% | MC-33 vents 1/4 open
Day 2 9% | MC-30
Day 3 20% | MC-24 unusually high rate of loss
Day 4 2% | MC-23
Day 5 7% | MC-21 closed vents a bit closer to 1/8 open
Day 6 4% | MC-19 cloudy/showers
Day 7 7% | MC-17
Day 8 6% | MC-16 vents now closed
Day 9 3% | MC-16 rain all day
Day 10 3% | MC-15 rainy day
Day 11 5% | MC-14 power out no fans
Day 12 9% | MC-12
Day 13 +3% | MC-13 rain/no fans - gained MC
Day 14 4% | MC-12
Day 15 9% | MC-11
Day 16 12% | MC-10 record heat starts
Day 17 5% | MC-9
Day 18 17% | MC-8
Day 19 +6% | MC-8.5 GAINED moisture

Some worthy-of-mentioning items ....

The last 4 days were as sunny and hot (touched
low 90's) as it gets here, and that weather
coming at the end of the drying cycle seems
to be the best case drying scenario I'm likely
to experience.

The first three days, moisture loss was very
fast (too fast), down to 24% - I find myself
wondering if this was due to the free water
being cooked off much more quickly then later
when the remaining moisture is mostly bound
water.

Things seemed to stall when the MC got to
the low 20's - up until the stall point, I
had the vents about a 1/4 open (aprox 100
sq/in of total open vent area). After reading
some of the Wood Doc's postings, I tried
closing the vents. Even fully closed, there's
likely 3-4 sq/in of opening around the vents
and door gap, and certainly some air leakage in
the structure, but I made a point of making the
kiln very tight (and very well insulated)
With the vents closed, moisture loss got closer
to the 10% target rate. Note to self: consider
closing the vents when MC reaches low 20's

The last couple of days, I took additional
MC readings using a pinless meter, and the
readings (after species correction and temp
correction at 1/4 inch depth) showed the
sample boards at 6% - even nudging high 5's
in some spots. I suspect that while the
weighing the sample boards is a necessity
at high MC's, as the lumber reaches final
MC, there may be some introduced error.
No matter - this kiln brought the load
down into (or very near) the 6 percent range.

I decided to leave the lumber in the kiln for
a bit to observe, and interestingly, the
MC rose the next day after the 6% reading.
I suspect there may be a point of "no returns
on investment" ... the lumber will hover
around 6%, and fluctuate based on outside
conditions - or perhaps any wetter pieces
are still drying a bit with the moisture
being picked up by the sample boards.

I'm going to post some responses that include
pictures and an interesting temp/humidity
measuring device.

Carl

7/15/18       #2: First solar kiln - structure pictur ...
Carl

Some pics of the kiln - the plan is to
stain it black when the board and batten
siding is dry.


View higher quality, full size image (1200 X 875)


View higher quality, full size image (1200 X 800)

7/15/18       #3: First solar kiln - kiln load pictur ...
Carl

I had a large piece of commercial rubber
roofing laying around, and use it as a
tarp to direct air flow through the pack,
and block air flow from wandering around
in other areas - it appears to be very
effective at getting good velocity through
the pack


View higher quality, full size image (1000 X 667)


View higher quality, full size image (1200 X 800)


View higher quality, full size image (1200 X 800)

7/15/18       #4: First solar kiln load - drying time ...
Carl

I found an inexpensive ($40) temperature/humidity
measuring device, and place the measurement
probes near the center of the pack.

The device has built in software that produces
timeline reports, and I've included the
report in PDF form. I marked it up to show
the MC of the sample pieces and the percentage MC loss for each day - the
report really gives insight to the daily
behavior of the kiln.

I bought a second one to monitor outside
conditions so I'd get some historical data
on performance at different times of year.

The recording device is:

Elitech GSP-6 Temperature and Humidity Data Logger Recorder

And can be purchased at Amazon:

https://www.amazon.com/gp/product/B01H3669T4/


View higher quality, full size image (900 X 801)


Click the link below to download the file included with this post.

20180703_kiln_run_report.pdf

7/15/18       #5: First solar kiln fans detail ...
Carl

I used three Lasko 20 inch fans, and made individual
fan mounts. With the roof lifted up to load,
the fan mounts tilt back against the back wall.

After the roof is lowered/closed, the fan mounts
are tilted against a stop strip on the bottom
of the rafters - I felt this tilted arrangement
might better direct the air move along the
collector rather then having them pointed
horizontally at the collector


View higher quality, full size image (600 X 900)


View higher quality, full size image (1200 X 800)


View higher quality, full size image (600 X 900)

7/15/18       #6: First solar kiln first load questio ...
Carl

After running the first load, I have some
questions I hope Gene can weigh in on...

1 - The fast rate of loss (too fast) when the
lumber was above 25-30% ... is this possibly
due to the kiln being more effective removing
free water moisture then bound water moisture?

2 - what type of degrade would one
expect when drying ash too fast early on
in the process (above, say, 20% MC)

3 - what would suggestions be for holding
cupping to a minimum? My first load had
almost no twist, bow, crook, and no end
checking, but there was quite a bit of cup.

It's worth noting that this first load was
"through sawn", and the worst cup
offenders were the pieces with juvenile
wood. The second load (in the kiln now)
was "grade sawn" with the associated
cants being left, and I'll be interested to
see how that effects overall cupping.

7/16/18       #7: First solar kiln load results ...
Gene Wengert-Wood Doc

1. I assume that you appreciate that the drying rate is based on the RH, velocity and temperature. With the vents open wide, plenty of air flow, and lots of sun, you will be able to dry the wood quite rapidly. Closing the vents a bit at the beginning, will slow down drying by raising the kiln humidity. The loss per day is the actual MC loss and not a percentage of that loss. So, 33% to 30% is a 3% loss and not 10% loss. So, you are not close to the maximum rate. The gain at the end might be because you are running the fans too much. Turn them On after the kiln has heated 10 F in the morning- -9AM ?- - and off around 7PM.

2. If you dry ash too fast, we might expect some minor cracking. You are not close to "too fast."

3. Cupping of wide pieces with the pith in or near is next to impossible. It is a natural event for wood. This cupping is a disadvantage of sawing "through and through" or live sawing. Slow drying encourages cupping.

7/16/18       #8: First solar kiln load results ...
Carl

Thanks Gene .... particularly the maximum
loss/percentage clarification ... sometimes
a little bit of knowledge can be a dangerous
thing.

It's obvious from your explanation that I
probably wont need to worry about drying
too fast with the size loads I'm putting in
the kiln, and your explanation:

"Slow drying encourages cupping."

Leads me to believe that it might be worth
experimenting with the size of the load,
reducing it until the drying rate approaches
the recommended maximum of 10+% for
ash.

All in all, it's been fun watching these first
two loads - me thinks one of the beauties
of your solar kiln design is that it's hard
for even the uninitiated to screw things up ;)

Carl

7/18/18       #9: First solar kiln load results ...
Matt Calnen

Gene, why does slow drying cause more cupping? I am a novice wood dryer. I have bought a couple of batches of lumber green from a farmer with a woodmizer and have not had trouble with what I would consider over cupping. Most of it was maple or ash, and 10” or less wide. I air dried the wood outside in a well stickered stack for two years that was covered on top, but the sides where open to the elements. I thought the wood came out good for what I paid. It had very little internal stress.

5/10/21       #10: First solar kiln load results ...
Jim Tomassino Member

Website: https://stuart.seacoastair.com/

Cupping of wide pieces with the pith in or near is next to impossible. It is a natural event for wood. This cupping is a disadvantage of sawing "through and through" or live sawing. Slow drying encourages cupping.

5/21/25       #11: First solar kiln load results ...
Daniel Member

Your detailed tracking and sample-based MC analysis was helpful to read—especially the adjustments to venting and timing of fan use. I’ve had similar results with ash stalling around 20%. The load-size adjustment idea is smart. Also curious how your grade-sawn load turned out in terms of cupping compared to the first. Any measurable improvement?


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • Baker Products
      Industrial Woodworking Machines, Wooden Pallet Manufacturing Machines, & Portable Sawmills
    • Rose Machinery
      Horizontal Band Re-rips, Standard & Custom Designed Machinery

    Become a Sponsor today!